1.0501 | 35 |
This grade is water-hardening steel suitable for small parts of moderate strength. Has moderate strength and hardness in the as-rolled condition, and can be strengthened and hardened by cold work. Machinability is only fair, as is weldability. Precautions must be taken when welding to avoid cracking from cooling too rapidly.
Composition:
%C | %Si | %Mn | %P | %S | Cr | Mo | Ni | other |
0,32-0,39 | ≤0,40 | 0,50-0,80 | 0,045 | 0,045 | ≤0,40 | 0,10 | ≤0,40 | Cr+Mo+Ni ≤0,63 |
Hot working:
Forging temperature range: 1100-850℃
Note: Heat to 1200 ℃. Do not forge below 850.
Heat treatment:
Soft annealing ℃ | HB 30-soft annealed | Normalizing ℃ | Hardening temperature for quenching in Water ℃ | Hardening temperature for quenching in Oil ℃ | Tempering temperature ℃ |
650-700 | 183 | 860-890 | 840-870 | 850-880 | 540-680 |
Main application:
Automobile- and motor construction
Shape of product:
Round, flat, step shape, ring, disc, shaft, other shape depend on customer needs