It is a martensitic stainless steels
Composition:
%C | ≤%Si | ≤%Mn | ≤%P | ≤%S | %Cr | ≤%Mo | %Ni | ≤%V | Nb | ≤% Others |
0,08-0.12 | 0.6 | 0.5 | 0.03 | 0.015 | 15-16.5 | 0.3 | 4-4.5 | 0.2 | 0.05-0.15 | 0.7 |
Hot working:
Forging temperature range: 1200-850℃
Note: Heat to 1200 ℃. Do not forge below 850.
Heat treatment:
annealing | Hardening temprature |
710-730 | 1030-1050 |
Main application:
Rang of application: stress corrosion cracking
Shape of product:
Round, flat, step shape, ring, disc, shaft, other shape depend on customer needs