1.7225 | 42 CrMo 4 |
This grade is generally suitable for heat treatment, constructional applications and similar uses.
Composition:
%C | %Si | %Mn | %P | %S | %Cr | %Mo | %Ni | % Other |
0,38-0,45 | 0,40 | 0.6-0.9 | 0,035 | 0,035 | 0,90-1,20 | 0.15-0.3 | – | – |
Hot working:
Forging temperature range: 1100-850
Note: Heat to 1200 ℃. Do not forge below 850.
Heat treatment:
Soft annealing ℃ | HB 30-soft annealed | Normalizing ℃ | Hardening temperature for quenching in Water ℃ | Hardening temperature for quenching in Oil ℃ | Tempering temperature ℃ |
680-720 | 248 | 840-880 | 820-850 | 830-860 | 540-680 |
Main application:
Bushes, arbors, control components, links
Shape of product:
Round, flat, step shape, ring, disc, shaft, other shape depend on customer needs