1.0570 | S355J2 |
St 52 steel is one of steel grade in DIN 17135. St 52 grades is used for Structural components and general purposes.
Grade, Class,
Type, Symbol or Name |
Steel
Number |
UNS Number | Heat Treatment | Section Thickness | Yield Strength, min | Tensile Strength, min
|
Elongation, min, % | Other | |||
t, mm | t, in. | N/mm2 or MPa | ksi | N/mm2 or MPa | ksi | ||||||
S355J2G3 | 1.0570 | — | N | < 3 | — | 355 | — | 510-680 | — | — | — |
3 ≤ t ≤ 16 | — | 355 | — | 490-630 | — | 20 | 27 J at -20°C | ||||
16 < t ≤ 40 | — | 345 | — | 20 | |||||||
40 < t ≤ 63 | — | 335 | — | 19 | |||||||
63 < t ≤ 80 | — | 325 | — | 18 | |||||||
80 < t ≤ 100 | — | 315 | — | 18 | |||||||
100 < t ≤ 150 | — | 295 | — | 470-630 | — | 18 | |||||
150 < t ≤ 200 | — | 285 | — | 450-630 | — | 17 | 23 J at -20°C |
Composition:
%C | %Si | %Mn | %P | %S | %Cr | %Mo | %Ni | % Others |
0.10-0.22 | 0,550 | 0.10-1.60 | 0,025 | 0,015 | 0.3 | 0.08 | 0.30 | Cr+Mo+Ni ≤ 0,0.48 |
Hot working:
Forging temperature range: 1200-850℃
Note: Heat to 1200 ℃. Do not forge below 850.
Heat treatment:
Soft annealing ℃ | HB 30-soft annealed | Normalizing ℃ | Hardening temperature for quenching in Water ℃ | Hardening temperature for quenching in Oil ℃ | Tempering temperature ℃ |
1100-850 | 650-700 | 223 | 850-880 | 820-850 | 830-860 |
Main application:
Structural components for general mech. Engineering
Shape of product:
Round, flat, step shape, ring, disc, shaft, other shape depend on customer needs