1.2436 X210CrW12

 

Very similar to X210Cr12 except has a tungsten addition giving it deeper hardening characteristics and enabling it to be hardened in air.

 

Composition:

 

%C %Si %Mn %P %S Cr W
2-2.3 0.1-0.4 0.3-0.6 Max0.03 Max0.03 11-13 0.6-0.8

 

Hot working:

Forging temperature range: 1170-850℃

Note: Heat to 1700 ℃. Do not forge below 850.
 
Heat treatment:

annealing ℃ Normalizing ℃ Hardening temperature ℃ Tempering temperature ℃
870 to 900 Do not normslize 980-1010 540

 

Main application:

Heavy duty cutting and punching tools, shear bladers, reamers.

Shape of product:

Round, flat, step shape, ring, disc other shape depend on customer needs